Knowledge Base

Articles

Pendulum Impact Testing Explained: Izod, Charpy, and Tension Impact

Overview

Pendulum impact testing is the most widely used method for measuring a material’s toughness. A weighted hammer is released from a known height, strikes a clamped specimen, and the energy absorbed at fracture is calculated from the height the pendulum rises to after impact. The result, expressed in joules, tells quality, R&D, and operations teams how a plastic, composite, ceramic, or non ferrous metal will behave under sudden shock loading. 

Three named techniques sit under the pendulum umbrella: Izod, Charpy, and tension impact. Each uses the same pendulum mechanics but a different specimen orientation, notch geometry, and clamping fixture. The Ray-Ran Advanced Pendulum Impact System performs all three on a single machine. 

How pendulum impact testing works

  1. Prepare the specimen. Machine the test sample to the dimensions and notch geometry required by the relevant standard. Notches concentrate stress at a predictable point, ensuring fracture initiates where it can be measured. 
  2. Clamp the specimen. Izod specimens are held vertically with the notch facing the striker. Charpy specimens are placed horizontally on supports with the notch facing away from the striker. 
  3. Release the pendulum. The hammer falls from a fixed, known height, gaining kinetic energy as it swings through the arc and strikes the specimen. 
  4. Measure the energy lost. Microprocessor controlled instruments calculate the difference between the pendulum’s pre impact and post impact height, expressing the result in joules. 
  5. Interpret the result. Higher absorbed energy indicates a tougher, more ductile material. Lower absorbed energy points to brittle behaviour. Repeat with multiple specimens to build a statistically valid dataset. 

Izod vs Charpy: the practical difference

Both Izod and Charpy strike a notched specimen with a swinging hammer and report the energy absorbed at fracture, but their setups differ in three ways: 

  • Specimen orientation – Izod is vertical and cantilevered, Charpy is horizontal and supported at both ends. 
  • Notch direction – Izod notches face the striker, Charpy notches face away from it. 
  • Application breadth – Charpy applies across a wider range of materials than Izod, and it is the better choice when a specimen fails through interlaminar shear or at the surface. 

Charpy testing is governed by ISO 179 (ISO 179-1 non instrumented, ISO 179-2 instrumented) and ASTM D6110. Izod testing is covered by ISO 180 and ASTM D256. 

Tension impact testing

Tension impact applies pendulum mechanics to a tensile loaded specimen, measuring the energy required to fracture a material under sudden pulling forces rather than bending. It is particularly useful for thin, brittle plastics that would deflect rather than break under a conventional Charpy or Izod blow. The Ray-Ran Advanced Pendulum Impact System supports tension impact testing using the specimen in bed method. 

Equipment and setup

A complete pendulum impact testing setup includes: 

  • A swinging hammer with interchangeable weights. The Ray-Ran system supports variable weight impact hammers up to 50 joules. 
  • Method specific fixtures – Izod vice, Charpy rest, tension impact rest, puncture impact fixture, pipe rest, and custom component fixtures. 
  • A microprocessor and software for result capture. Ray-Ran ships Techni-Test Windows software, with CSV export to Excel. 
  • Safety enclosure – a full guard around the pendulum arc. 
  • Optional low temperature chamber for evaluating ductile to brittle transition behavior. 

Common errors and best practice

  • Inconsistent notch geometry. Notch depth, angle, and tip radius materially affect results. Always use a calibrated notch cutter and verify against the standard. 
  • Temperature drift. Plastics are temperature sensitive. Condition specimens to the standard’s specified temperature before testing. 
  • Insufficient sample size. Single results are unreliable. Test the number of specimens required by the standard and report mean and standard deviation. 
  • Wrong fixture for the material. Use Charpy for surface effect or shear failure modes, Izod for clean comparative data on rigid plastics, and tension impact for thin or brittle specimens that deflect rather than break. 

Choosing the right Ray-Ran impact tester

Material / sample  Standard  Recommended Ray-Ran instrument 
Rigid plastics, composites, ceramics  ISO 179, ISO 180, ASTM D6110, ASTM D256  Advanced Pendulum Impact System 
Pipes and large diameter sections  ISO 3127, EN ISO 11173  Falling Weight Impact Tester 
Thin plastic films  ASTM D1709, ASTM D4272, ISO 7765-1  FDT-A2 RR-FDT-A2 Advanced Floor Mounted Falling Dart Tester 
Entry level film impact testing  ASTM D1709 Method A (Method B with extension pack)  Manual Basic Falling Dart Impact Tester 

+ Manual Advanced RR-FDT-MA 

Was this useful?

FAQs

  • Both Izod and Charpy use a swinging pendulum to fracture a notched specimen and measure absorbed energy in joules. The difference is setup. Izod clamps the specimen vertically with the notch facing the striker. Charpy supports the specimen horizontally with the notch facing away. Charpy is the more versatile of the two, and it is preferable when failure starts from shear or at the surface. Izod is governed by ISO 180 and ASTM D256, Charpy by ISO 179 and ASTM D6110. 

  • The primary standards are ASTM D1709 (Method A uses a 38.1mm dart from 66cm; Method B uses a 50.8mm dart from 1.5m), ASTM D4272 (total energy by kinetic energy lost), and ISO 7765-1. The FD-A2 Advanced Floor Mounted Falling Dart Tester from Ray-Ran complies with all three plus ISO 6603. 

  • Composite plate impact testing is governed by ASTM D7136, which specifies a drop weight test using a 16mm hemispherical impactor and potential energy of 6.7J multiplied by specimen thickness.  

  • Instrumented impact testing fits a striker with strain gauged loadcells and velocity sensors that record the full force, velocity, energy, time, and displacement curve through the impact event. Standard pendulum or drop weight tests only report a single absorbed energy figure. Use an instrumented system when you need to identify the exact point of damage initiation, characterise progressive failure, or comply with ISO 6603 or ASTM D3763. 

  • The Ray-Ran Advanced Pendulum Impact System performs Izod, Charpy, and tension impact testing on a single machine. It supports variable weight hammers up to 50 joules, ships with Techni-Test Windows software for CSV export, includes an optional safety enclosure, and accepts an optional low temperature chamber for ductile to brittle transition work. 